Abstract
Global climate change is accompanied by a change in tree composition in many regions. In Europe, the distribution areas of many species are expanding towards the north so that, among others, black locust (Robinia pseudoacacia), which is native to the USA and has long been established in south-eastern Europe, is also becoming increasingly important in central and northern Europe. Many other tree species are known to have different properties between their original and new locations, including the biological durability of the wood. Hence, the resistance of black locust wood against decay fungi was studied concerning origin-specific differences. Wood was sampled from seven different origins in Europe and original habitats in the United States. Fungal incubation experiments were conducted, wood extractives were analysed, and different anatomical characteristics were quantified such as ring width, vessel size distribution and the presence of tyloses. In addition to differences in durability between juvenile and mature wood, origin-specific differences within the mature heartwood were attributed to extractive contents and the percentages of earlywood vessels containing tyloses. Based on parameters that contributed at least 20% to mass loss, susceptibility to fungal decay was modelled with multiple regressions.
Similar content being viewed by others
Avoid common mistakes on your manuscript.
Introduction
Climate change influences the range of suitability for commercially important tree species (Briscoe et al. 2023; Hama and Khwarahm 2023). Progressive forest management is looking to wood species that are robust to the potential changes in growth conditions. Climate change may influence wood properties, which means that wood properties and performance will change over time in original habitats, and that they may differ between traditional and evolving habitats. Some of the candidate species considered for use in construction show high biological durability and may also serve for outdoor building applications, such as European oak (Quercus robur & Q. petraea) and sweet chestnut (Castanea sativa), which are becoming increasingly available (Conedera et al. 2016; Eaton et al. 2016). There is high demand for European white oaks. While they are well established in Central Europe, their growth and spread potential is increasing in the Nordic countries, such as Norway and Sweden. But other ring-porous hardwood species of higher durability may be seen as alternatives in Central Europe, since they are supposed to better cope with droughts and calamities than the established species. Among them, we find sweet chestnut (Freitas et al. 2022; Conedera et al. 2021) and black locust (Robinia pseudoacacia) (Bedbur et al. 2010). The latter is addressed in this study.
Black locust, also called yellow locust, has a disjunct original range in the United States (Huntley 1990). The eastern section is centred in the Appalachian Mountains and ranges from central Pennsylvania and southern Ohio south to north-eastern Alabama, northern Georgia, and south-western South Carolina. The western section ranges from southern Missouri to northern Arkansas and north-eastern Oklahoma. However, black locust has been planted widely and became naturalized throughout the United States, Canada, Europe and Asia (Huntley 1990; Sitzia et al. 2016; Puchałka et al. 2021). It is considered the first North American tree species imported to Europe in the early 17th century and was named after Jean Robin, the gardener of King Henri IV of France, who planted the first trees in Paris (Demené and Merzeau 2007).
Black locust was extensively planted in Central Europe. It is nowadays widespread and the most used non-native tree species on the continent (Brus et al. 2019). Furthermore, black locust is considered a ‘climate change winner’ tree species since it tolerates drought and nutrient poor soils (DeGomez and Wagner 2001) and is therefore of increasing interest in reforestation. However, black locust mostly regenerates vegetatively by root suckers and may therefore be considered invasive (Vítková et al. 2017). Thus, its suitability for replacement of less drought-tolerant European tree species is debated (Li et al. 2014; Dyderski et al. 2018; Nicolescu et al. 2018; Nadal-Sala et al. 2019; Puchałka et al. 2021).
The wood of Robinia pseudoacacia is highly valued and has been appreciated for many different purposes (Cuno 1930; Huntley 1990; DeGomez and Wagner 2001; Page et al. 2013; Vítková et al. 2017).
The durability of the ring-porous heartwoods is a function of water exclusion efficacy, e.g. through the formation of tyloses, and the presence of biologically active secondary metabolites (Ruppitsch et al. 2021). Intra-species variability of moisture dynamics in black locust were reported by Brischke et al. (2024). The high natural durability of black locust heartwood is often explained by the presence of bioactive phenolic extractives (Pollet et al. 2008; Latorraca et al. 2011). Extractives from black locust heartwood include radical scavengers (Vek et al. 2020a, b; Hosseinihashemi et al. 2016). It is assumed that non-enzymatic antioxidants have an important inhibitory effect against brown rot fungi. Free radicals produced in the first, oxidative radical-based phase of the two-step wood degradation mechanism of brown rots are scavenged by the antioxidant extractives (Belt 2022, Schultz et al. 2000). Triterpenes and simple sugars (e.g., sucrose, glucose and fructose) and non-structural carbohydrates (starch); soluble proteins and phenolic compounds such as simple phenols, phenolic acids, stilbenes, flavonoids and condensed tannins have been identified in the tissues of black locust. Flavonoids dihydrorobinetin (flavanonol), robinetin (flavonol) and derivates of hydroxycinnamic acid have been reported to be the characteristic phenolic compounds present in the hydrophilic extracts of black locust heartwood (Vek et al. 2019a, b). The high natural durability of the heartwood of black locust is also explained by the presence of dihydrorobinetin and robinetin in these tissues (Magel et al. 1994; Sergent et al. 2014). Similar compounds are reported for oak and sweet chestnut (Eichhorn et al. 2017).
The density of ring-porous hardwoods increases with increasing ring width. It has also been reported that the durability of English oak (Q. robur) with extremely narrow rings is relatively low, similar to the durability of European beech (Fagus sylvatica) (Humar et al. 2008).
The content of heartwood extractives depends also on the position in the stem. It was demonstrated that the heartwood of black locust is characterized by well-defined radial variability, whereas the amount of extractives significantly decreases from the outermost heartwood towards the pith (Magel et al. 1994; Dünisch et al. 2010; Latorraca et al. 2011; Vek et al. 2020b). The axial variability of the extractive content in black locust stemwood is less pronounced (Adamopoulos et al. 2005). The extractives in black locust stemwood have been relatively well studied, but there is little data on the fungal decay resistance of black locust heartwood of different ages.
Wood species can be assigned to five durability classes (DC) of biological durability against wood-destroying fungi (DC 1 ‘very durable’ to DC 5 ‘non-durable’) according to EN 350 (2016). Black locust is assigned to DC 1–2 (1–2), where the classes refer to tests with soil contact and with basidiomycetes (in parentheses) respectively. For some wood species, DCs refer also to different origins, e.g., Douglas-fir (Pseudotsuga menziesii) from North America or those cultivated in Europe (EN 350 2016). Previous studies indicate that similar differences can be expected also for black locust and other hardwoods with coloured heartwood (Adamopoulus et al. 2005, Brischke et al. 2009; Dünisch et al. 2010; Meyer et al. 2014; Eichhorn et al. 2017). In particular, the juvenile wood percentage and the amount and composition of extractives with inhibitory effect on fungal growth differs between origins. Differences in durability between sources from original stands and evolving habitats or plantations were reported, for instance for teak (Tectona grandis) and Western red-cedar (Thuja plicata) (Haupt et al. 2003; Stirling et al. 2012). However, the effect of climate and other site-specific effects on the biological durability of European-grown ring-porous hardwood species such as black locust is neither fully understood nor quantified in terms of durability classes or service life expectancies.
The aim of this study was to examine whether the biological durability of black locust varies by origin and to identify potential wood-specific parameters that impact the material-inherent resistance against decay fungi. For this purpose, black locust wood was sampled from different origins in Europe, and from its native range in the United States. Fungal incubation experiments were conducted, wood extractives were analysed, and different anatomical characteristics were quantified such as ring width, vessel size distribution and the formation of tyloses.
Materials and methods
Wood material
Black locust (Robinia pseudoacacia) stem sections originating from two to five trees per study region were investigated (Table 1). The origin could only be traced back to the regional level. Stem sections were cut into planks using a band saw and air-dried at the University of Goettingen. Specimens were sampled from central boards at different zones of the stem, i.e., in the outer heartwood (adjacent to the sapwood, hwouter), the central heartwood (hwcentral), and the inner heartwood (juvenile wood, hwinner) as shown in Fig. 1. Juvenile wood specimens were taken within the inner 15 annual rings; the pith itself was excluded. Material from three regions in the United States was sawn board sections, partly without pith, and therefore pooled as shown in Table 1.
For an additional consideration of the entire heartwood (hwtotal), the data for the three previously separately considered heartwood sections were pooled. Specimens of 15 × 25 × 50 (ax.) mm³ were made from central boards of each stem section. Virulence control specimens were made from Scots pine (Pinus sylvestris) sapwood and European beech (Fagus sylvatica).
Durability tests with basidiomycetes
The durability of the different black locust timbers was evaluated according to EN 113-2 (2021). Therefore, two to 38 replicate specimens were used for each combination of test fungus, origin, and stem zone. The number of replicates varied due to varying availability of the test material.
Virulence control specimens were made from Scots pine sapwood and European beech. The following fungal strains were used for the tests: the brown rot fungus Coniophora puteana = (Schum.:Fr.) P. Karsten BAM Ebw. 15 and the white rot fungus Trametes versicolor = (L.:Fr.) Pilat CTB 863 A.
Before incubation for 16 weeks, the test specimens were conditioned at 20 °C / 65%RH to constant mass, weighed to the nearest 0.001 g, steam sterilized in a steam pot for 20 min and another 10 min on the following day. Afterwards, sets of two specimens of the same combination of wood species, origin, and stem section were placed on fungal mycelium in Kolle flasks filled with 100 ml malt extract agar (4%). Additional moisture content control specimens were oven-dried at 103 ± 2 °C. Their average equilibrium moisture content (EMC) was used to calculate the theoretical initial oven-dry mass of all test specimens according to EN 113-2 (2021).
After incubation, the specimens were cleaned of adhering mycelium, weighed to the nearest 0.001 g, oven-dried at 103 ± 2 °C, and weighed again. The ML of the specimens were determined and median ML was used to assign durability classes (DC) between DC 1 (very durable) and DC 5 (not durable) according to EN 350 (2016).
Anatomical analysis
The anatomical analysis included measuring the dimensions of vessels and the analysis of tylosis-bearing vessels within the samples of Robinia pseudoacacia from different wood origins (Table 1). Before image collection, specimens with the size of 15 × 25 × 50 (ax.) mm³ were prepared according to EN 113-2 (2021), and then cut into smaller specimens with cross-sectional surfaces of 12.5 × 15 mm2 (R×T). Subsequently, the surface of these specimens was smoothed using a microtome. The image collection was performed using the digital 3D reflected light microscope Keyence VHX-7000 (Keyence, Neu-Isenburg, Germany). The Keyence VHX-7000 (VHX) allows to obtain true-colour images of the observation surface non-destructively. All images were acquired at a lens magnification of 100× and saved as TIFF files. Each saved image was the result of several 2D images stitched together into a composite image. Using VHX composite images, the entire sample surface was captured.
The image analysis was performed by the open-source GIMP software (GIMP Development Team). Prior to the analysis, the pixel size of the images was set in GIMP based on the pixels of their scale bars. For each cross-section, three rectangular boxes, whose size radially covered one annual ring and tangentially 2000 μm, were extracted for the analyses as indicated in Fig. 2. Within these boxes four anatomical traits were considered for earlywood and latewood: (i) the number of vessels, (ii) the radial diameter of vessel lumina, (iii) the percentage of vessels containing tyloses, and (iv) the width of earlywood and latewood. Vessels smaller than 10 μm in diameter were not considered. The examinations were performed for the different growing locations, stem sections (i.e., outer heartwood (hwouter) and inner heartwood (hwinner) zones, and annual ring zones (i.e., earlywood and latewood).
Extraction and chemical analysis
Extraction
Prior to extraction and chemical analyses, blocks of black locust heartwood were ground with a Retsch SM 2000 cutting mill using a 1 mm bottom sieve. The ground samples were freeze-dried for 24 h at -85 °C and 4.5 kPa in a Telstar LyoQuest CC1930 lyophilizator, weighed into the 10 mL SST extraction cells, and extracted in a Thermo Scientific™ Dionex™ ASE™ 350 Accelerated Solvent Extractor. Accelerated extraction was performed with aqueous acetone (90%, v: v) at 110 °C and 10.342 MPa. One gram (dw) of the heartwood sample was extracted with 4 × 5 min static cycles under nitrogen. Final volumes of the acetone heartwood extracts were defined to 100 mL.
Gravimetrical analysis
Total hydrophilic extractives (THE) were determined gravimetrically. Aliquots of heartwood extracts were dried in an oven to constant weight using a temperature gradient from 60 °C to 105 °C. THE were measured in milligrams per gram of dry heartwood sample (mg/g, dw) (Vek et al. 2019a). The results of the gravimetric analysis are expressed as a percentage of THE per dry weight of the sample (% w/w, dw).
Spectrophotometric analysis
Total phenol contents (TPC) in heartwood samples were measured according to a protocol previously described by Singleton and Rossi (1965) and Vek et al. (2019a). Briefly, aqueous Folin–Ciocalteu phenol reagent (diluted 10 times) and aqueous solution of sodium carbonate (75 g/L) were added to 0.25 mL of a heartwood extract. After incubation of the reaction mixtures, absorbance was measured at 765 nm using a Perkin-Elmer UV/Vis spectrophotometer. The results were expressed in milligrams of gallic acid equivalents per gram of dried wood sample (mg GAE/g dw). The method for semi-quantitative determination of TPC was linear in the selected concentration range (R2 > 0.99).
HPLC analysis
Reference compounds in black locust heartwood, i.e., dihydrorobinetin (DHR) and robinetin (Rob) were measured with a high-performance liquid chromatography system equipped with a photodiode array detector (Thermo Scientific, Accela 600 HPLC-PDA) (Vek et al. 2022). Samples were separated on a Thermo Accucore C18 column with dimensions of 4.6 mm (I.D.) × 150 mm, particle size of 2.6 μm). Water + 0.1% formic acid (v/v) (A) and methanol + 0.1% formic acid (v/v) (B) served as a mobile phase. The flow rate of the mobile phase was 1 mL/min. The gradient used was from 5 to 95% of solvent (B). The temperature of an auto-sampler with sample trays and the temperature of a column oven were 5 and 30 °C, respectively. Analytical HPLC standards for DHR and Rob were purchased from Extrasynthese (HPLC assay, ≥ 95%). Absorbance of separated compounds of heartwood extracts and those of HPLC standards were measured at 280 nm and UV spectra were recorded from 200 nm to 400 nm. The calibration curves for DHR and Rob used for quantitative analysis were linear (R2 > 0.99).
Antioxidant assay
After the chemical analyses, the heartwood extracts of the same growth site were pooled. Eleven samples of black locust heartwood, one sample per site (Table 1), were prepared. The extracts were dried using a vacuum chamber (at 10 kPa and room temperature), lyophilizator (same conditions as described above) and then re-dissolved in water. Gallic acid (GA) and ascorbic acid (AA) were used as reference antioxidants. The 2,2-diphenyl-1-picrylhydrazyl (DPPH) radical scavenging activity was measured according to the protocol described by Vek et al. (2020a). Briefly, the references and the heartwood extracts were prepared in ten testing concentrations (1000 mg/L – 1,6 mg/L). Water and methanol were used as a control. A 2.25 mL of DPPH methanol solution was mixed with a 90 µL of sample. The reaction mixtures were incubated for 30 min in the dark at room temperature. After incubation, the reduction of DPPH radical was determined colorimetrically by measuring absorbance at 517 nm with UV-Vis (see above). Results are expressed as DPPH radical scavenging activity (%RSA), together with the IC50 (50% inhibition concentration, mg/L).
Statistical analysis
Each combination of origin and stem zone was one group of statistical interest. The two preconditions normal distribution (Shapiro-Wilk test) and homogeneity of variances (Levene test) were checked first. Depending on the results, the compatible tests for further analysis were chosen. If there were more than two groups to compare (e.g., decay tests and the chemical analysis) an omnibus-test (analysis of variance, Welch or Kruskal-Wallis test) and the compatible post-hoc analysis (Tukey, Games Howell or Steel-Dwass test) were applied to do pairwise comparisons. Only two stem zones were considered per origin for analysis of anatomical features (see sect. Anatomical analysis). Hence, different tests were used for their analysis (i.e., t-test, Mann-Whitney test). Multiple or multifactorial regressions were conducted to examine which extractives had an influence on mass loss by fungal decay (see sect. Multifactorial analysis of impact variables).
The chemical structures of flavonoids and stilbenes presented with figures were prepared by using a Perkin Elmer’s ChemDraw 20.1 software.
Results and discussion
Mass loss by fungal decay
Mass loss (ML) of black locust heartwood by fungal decay differed between stem sections, test fungi and wood origins (Fig. 3). Generally, the white rot fungus T. versicolor caused higher ML on black locust, compared to the brown rot fungus C. puteana, which coincides with the general association of white rot fungi and hardwoods. T. versicolor was generally more virulent than C. puteana (Table 2), but both test fungi caused ML well above the threshold of 20%, and C. puteana even well above 30%. Hence, the test was valid according to EN 113-2 (2021).
The ML data and the corresponding DCs are shown in Fig. 3 and Table 3 and do basically coincide with the durability classification provided by EN 350 (2016), i.e., DC 1–2 (1–2). The median ML of both the inner and central black locust heartwood of all origins was below 5% except for the material from Calw in south-western Germany (Fig. 3). The latter showed a median ML of 6.4% (hwouter) and 14.3% (hwcentral) after incubation with T. versicolor and should therefore be assigned to durability class (DC) 2 and 3, respectively (EN 350 2016). Furthermore, the hwcentral from Sibiu (Romania) had a median ML of 5.01% and was thus assigned to DC 2. Black locust from all other origins was assigned to DC 1 (≤ 5% ML) including the wood from the US. T. versicolor caused small differences in ML between the different heartwood groups.
Larger differences in ML between the origins were found for the inner heartwood specimens of black locust (Fig. 3). The highest median ML caused by T. versicolor was obtained for inner heartwood from Calw (23.2%) followed by that from Reinhausen (22.6%), Sibiu (7.7%) and Brandenburg (5.7%). The lowest median ML was determined for inner heartwood from the Alsace (4.0%). The generally lower durability of the inner heartwood, which is likely juvenile wood, was expected and confirms previous findings, e.g., by Dünisch et al. (2010) who found 17% ML of juvenile wood, while mature heartwood had only 1.7% ML both caused by T. versicolor.
Anatomical traits
Inner and outer heartwood differed visibly in their anatomical traits, such as ring width, and number and diameter of vessels (Table 4). On average for all wood origins, the annual tree-ring width was 2.8 mm for the outer heartwood (hwouter) and 4.5 mm for the inner heartwood (hwinner, Table 4). In other words, the ring width of hwinner was 1.6 times of that of hwouter. Unlike the similar width of the earlywood zone in both heartwood sections (approx. 0.6 mm), the widths of the latewood zones differed considerably. This consistency of earlywood, and the variation in latewood is typical for ring-porous hardwoods (Carlquist 2013). Thereby, the latewood width of 3.8 mm for hwinner was 1.8 times of that for hwouter (width of 2.1 mm). Even though the hwinner tended to larger ring widths for most of the locations, stems from Dolsko and Calw showed marginally greater ring widths for hwouter. Previous studies (Adamopoulos et al. 2010; Adamopoulos and Voulgaridis 2002; Dünisch et al. 2010) showed that the tree-ring widths of black locust decrease with cambial age in the first 20 years distinctly.
The wood of black locust showed a typical ring-porous vessel distribution (IAWA Committee 1989; Wagenführ 1999; Table 5). In this study, earlywood vessels in hwinner and hwouter were two and three times larger than latewood vessels (Table 4). Average earlywood vessel size of hwinner, (105 μm) was greater than that of hwouter (90 μm). However, comparing the earlywood and latewood separately, an opposite trend became obvious. The earlywood vessels were marginally smaller in the inner heartwood zone than those in the outer heartwood zone (Table 3). An opposite trend was observed for latewood vessels (Table 5).
Because of the small size of latewood vessels and the large width of latewood sections, it was not surprising that the number of vessels in the latewood was considerably higher compared to the earlywood (Table 4). Unlike the number of earlywood vessels, which was similar for all origins, the number of latewood vessels varied between origins from 20 in Brandenburg to 139 in Dolsko.
Black locust is known as a hardwood species with a high rate of vessel occlusions (i.e., tyloses) of heartwood. That fact was confirmed in this study. Regarding the vessels without tyloses, there was no significant difference between the heartwood zones (Table 4) with average values of 26% and 23%, respectively. Within the growth rings, the highest rate of tyloses in vessels was found in earlywood. Here, only 6% of the vessels were free of tyloses. In latewood, 27% of vessels were free of tyloses. It should be noted that the examination of vessel occlusion was accomplished on 2D microscopy images. Vessels that revealed no tyloses during the 2D examination, however, might be occluded by tyloses elsewhere within the same vessel.
Content of extractives
The chemical analysis revealed significant differences in the amounts of total hydrophilic extractives (THE) among the heartwood samples of different geographical origins (ANOVA, p = 0.01) (Table 6). The highest amounts of THE were extracted from the heartwood samples from northern Alabama followed by Alsace, Celle, Dolski, Sibiu, western Tennessee, and Calw. The results of the gravimetric analysis are supported by the results of the colorimetric analysis, which also showed significant differences in total phenol contents (TPC) among the heartwood samples examined (ANOVA, p < 0.01, Table 6). The largest TPC were measured in heartwood samples from northern Alabama (51.84 mg/g) and Alsace (36.31 mg/g) (LSD test). In contrast, the lowest TPC was characteristic for samples from Calw (20.07 mg/g) (LSD test). It has already been demonstrated that the heartwood of black locust is characterized by a significant radial gradient in extractive content with higher amounts of THE, TPC and DHR in the outermost heartwood (Vek et al. 2020b). In the present study, a significant decrease of THE, TPC and DHR in the centripetal direction (hwouter → hwcentral → hwinner) was also found for black locust heartwood of other geographical origins (ANOVA, pTHE, TPC, DHR, Rob > 0.051). On average, the hwouter contained significantly higher amounts of THE, TPC, DHR, and Rob than the juvenile hwinner (LSD test, Fig. 4).
The applied HPLC method has already been demonstrated to be efficient for the chemical monitoring of dihydrorobinetin (DHR) and robinetin (Rob) in wood and bark extracts of black locust (Vek et al. 2019b, 2020b; Keržič et al. 2023). The most abundant and characteristic peak on the HPLC chromatograms was assigned to DHR (Fig. 4). Besides DHR and also other identified compounds that are extracted from wood of black locust (Sanz et al. 2012), Rob is referred to be one of the characteristic flavonoids (Sergent et al. 2014; Bostyn et al. 2018; Atwi-Ghaddar et al. 2023). The stilbenes piceatannol and resveratrol were also found in the heartwood samples but only in traces (Fig. 4). However, DHR and Rob are related to the higher decay resistance of black locust heartwood (Smith et al. 1989; Rademacher et al. 2016). The HPLC showed significant differences in the content of DHR in Rob in the investigated heartwood samples (ANOVA, pDHR, Rob > 0,051) (LSD test). On average, among the trees of investigated geographical regions, the heartwood of black locust from Dolsko and Brandenburg contained the highest amounts of DHR, while heartwood from Reinhausen was the richest in Rob (Table 1; Fig. 4).
The protective role of phenolic extractives against wood decay is explained also with nonbiocidal properties, e.g., with their free radical scavenging activity (Schultz et al. 2002), and extractives of black locust have already been demonstrated to be good natural antioxidants rather than fungal growth inhibitors (Vek et al. 2020a, b). Hence, a preliminary analysis was performed and the 2,2-diphenyl-1-picrylhydrazyl (DPPH) radical scavenging activity (RSA) of heartwood extracts of different geographical origin was measured. The results of the antioxidant assay are presented as IC50 values (Fig. 5), i.e., with the concentration of a heartwood extract that scavenges 50% of the initial DPPH radicals, and with the plots showing DPPH radical scavenging activity regarding the test concentration of the heartwood extract.
Comparison of DPPH RSA to those of reference natural antioxidants, i.e., gallic and ascorbic acid, showed that the tested heartwood extracts are good free radical scavengers (Fig. 5). Heartwood extracts at 250 mg/L showed DPPH RSA around 80% or even higher. The tested heartwood extracts performed well as natural antioxidants also at the lower test concentrations. For example, heartwood extracts at 100 mg/L from northern Alabama, Brandenburg, Alsace and Reinhausen showed RSA comparable with the RSA of ascorbic acid of the same concentration. Heartwood extract of black locust from Dolsko at 100 mg/L was an even better scavenger of free radicals than ascorbic acid. Almost the same DPPH RSA number has been reported for the heartwood extracts of black locust that were sampled at the suburban forest Panovec near Nova Gorica, Slovenia (Vek et al. 2020a; Fig. 5). An average concentration of the heartwood extracts that scavenge 50% of the initial DPPH radicals, was measured to be 162.9 mg/L. IC50 values for gallic acid and ascorbic acid were 49.5 and 133.0 mg/L. Phenolic compounds are believed to protect the wooden cell wall after a fungal attack by scavenging free radicals produced by the Fenton reaction (Schmidt 2006; Schultz et al. 2000, Valette et al. 2017). In summary, the results of the chemical analysis showed that the geographical origin has an important influence on both the content of extractives and the antioxidant properties of the heartwood extracts of black locust.
Multifactorial analysis of impact variables
Possible influences of the chemical and anatomical parameters on the fungus-induced ML were investigated. Therefore, stem sections per fungus were differentiated first, followed by further differentiations in a second run. The interrelationships between ML by fungal decay and the content of total hydrophilic extractives (THE), total phenols (TPC), dihydrorobinetin (DHR), and robinetin (Rob) separately are shown in Figs. 6 and 7. It became evident that these parameters were better correlated with ML by T. versicolor compared to those caused by C. puteana, which was also generally lower in ML values. The best correlation was obtained between ML by T. versicolor and THE, followed by TPC, DHR, and Rob which coincided with previous findings by Vek et al. (2020), who showed the variability of extractives in black locust stems with gradients from hwouter to hwinner. The lower decay resistance of the juvenile wood of black locust might be attributed to extractive gradients, but the latter became evident also within one stem zone (Figs. 6 and 7). In contrast to the extractives, the ML was barely influenced by the percentage of vessels closed with tyloses.
The results of a predictor screening, where THE, TPC, DHR, Rob and the percentage of different vessels without tyloses were checked all together, are summarized in Table 7. Differences in contributions between the single stem sections and the total stem are partly explained by the lack of information for hwcentral. The parameters, that contributed at least 20% to the ML, were in case of both ML by T. versicolor and ML by C. puteana TPC and THE. Due to the small number of replicates, potential interactions between the parameters remained unconsidered. We got the following two linear models:
and calculated the theoretical values for ML with these formulas, Table 7. The measured and predicted ML were compared in Fig. 8.
Again, it became clear that the relationships between the influencing variables and the resulting ML were more pronounced for T. versicolor compared to C. puteana. Generally, the fit between predicted and measured ML was surprisingly striking.
Conclusion
The results of this study made clear that the biological durability of the black locust heartwood is subject to considerable variability. Black locust from most origins was assigned to DC 1 including the wood from the US, but wood from Calw (Germany) was assigned to DC 2 and 3, material from Sibiu (Romania) to DC 2. These differences could partly be attributed to the origin of the test material and associated differences in the extractive content of the wood. The influence of vessels blocked by tyloses was negligible. In general, the results obtained are indicative, since the underlying sample size was limited. Future studies with a larger sample size and considering further wood origins are needed to validate the recent findings. Nevertheless, the influence of the most important influencing variables could be quantified and used for a simple prediction model of ML with a surprisingly high level of accuracy. Increased understanding of source-associated variability in wood durability will be helpful as forest management and climate change alter the distribution of useful tree species.
Data availability
Data are available from the authors on request.
References
Adamopoulos S, Voulgaridis E (2002) Within-tree variation in growth rate and cell dimensions in the wood of black locust (Robinia pseudoacacia). IAWA J 23:191–199. https://doi.org/10.1163/22941932-90000297
Adamopoulos S, Voulgaridis E, Passialis C (2005) Variation of certain chemical properties within the stemwood of black locust (Robinia pseudoacacia L). Holz Roh- Werkst 63:327–333. https://doi.org/10.1007/s00107-005-0018-3
Adamopoulos S, Passialis C, Voulgaridis E (2010) Ring width, latewood proportion and density relationships in black locust wood of different origins and clones. IAWA J 31:169–178. https://doi.org/10.1163/22941932-90000014
Atwi-Ghaddar S, Destandau E, Lesellier E (2023) Optimization of supercritical fluid extraction of polar flavonoids from Robinia pseudoacacia L. heartwood. J CO Util 70:102440. https://doi.org/10.1016/j.jcou.2023.102440
Bedbur I, Matthes U, Konold W (2010) Pionierbaumarten – Chancen, Verbreitung und Potenziale im Klimawandel in Rheinland-Pfalz. [Pioneer tree species – Chances, distribution, and potential during climate change in Rhineland-Westphalia. Forst Holz 65:20–27
Belt T, Harju A, Kilpeläinen P, Venäläinen M (2022) Fungal degradation of extractives plays an important role in the brown rot decay of Scots pine heartwood. Front Plant Sci 13:912555. https://doi.org/10.3389/fpls.2022.912555
Bostyn S, Destandau E, Charpentier J-P, Serrano V, Seigneuret J-M, Breton C (2018) Optimization and kinetic modelling of robinetin and dihydrorobinetin extraction from Robinia pseudoacacia wood. Ind Crops Prod 126:22–30. https://doi.org/10.1016/j.indcrop.2018.09.049
Brischke C, Welzbacher CR, Rapp AO, Augusta U, Brandt K (2009) Comparative studies on the in-ground and above-ground durability of European oak heartwood (Quercus petraea Liebl. and Quercus robur L). Eur J Wood Prod 67:329–338. https://doi.org/10.1007/s00107-009-0329-x
Brischke C, Purps H, Emmerich L (2024) Intra-species variability of moisture dynamics in wood. IRG/WP 24-11040. The International Research Group on Wood Protection
Briscoe NJ, Morris SD, Mathewson PD, Buckley LB, Jusup M, Levy O, Maclean IMD, Pincebourde S, Riddell EA, Roberts JA, Schouten R, Sears MW, Kearney MR (2023) Mechanistic forecasts of species responses to climate change: the promise of biophysical ecology. Glob Change Biol 29:1451–1470. https://doi.org/10.1111/gcb.16557
Brus R, Pötzelsberger E, Lapin K, Brundu G, Orazio C, Straigyte L, Hasenauer H (2019) Extent, distribution and origin of non-native forest tree species in Europe. Scand J Res 34:533–544. https://doi.org/10.1080/02827581.2019.1676464
Carlquist S (2013) Comparative wood anatomy: systematic, ecological, and evolutionary aspects of dicotyledon wood. Springer Science & Business Media, Berlin
Conedera M, Tinner W, Krebs P, de Rigo D, Caudullo G (2016) Castanea sativa in Europe: distribution, habitat, usage and threats. In: San-Miguel-Ayanz J, de Rigo D, Caudullo G, Durrant H, Mauri T, A. (eds) European Atlas of Forest Tree Species. Publ. Off. EU, Luxembourg
Conedera M, Krebs P, Gehring E, Wunder J, Hülsmann L, Abegg M, Maringer J (2021) How future-proof is Sweet chestnut (Castanea sativa) in a global change context? Ecol Manag 494:119320. https://doi.org/10.1016/j.foreco.2021.119320
Cuno JB (1930) Utilization of black locust, vol 131. US Department of Agriculture, Washington, DC
DeGomez T, Wagner MR (2001) Culture and use of black locust. HortTechnol 11:279–288. https://doi.org/10.21273/HORTTECH.11.2.279
Demené JM, Merzeau D (2007) Black locust. History and biological characteristics. Forêt-entreprise 177:10–12
Dünisch O, Richter HG, Koch G (2010) Wood properties of juvenile and mature heartwood in Robinia pseudoacacia L. Wood Sci Technol 44:301–313. https://doi.org/10.1007/s00226-009-0275-0
Dyderski MK, Paź S, Frelich LE, Jagodziński AM (2018) How much does climate change threaten European forest tree species distributions? Glob Change Biol 24:1150–1163. https://doi.org/10.1111/gcb.13925
Eaton E, Caudullo G, Oliveira S, de Rigo D (2016) Quercus robur and Quercus petraea in Europe: distribution, habitat, usage and threats. In: San-Miguel-Ayanz J, de Rigo D, Caudullo G, Houston Durrant T, Mauri A (eds) European Atlas of Forest Tree Species. Publ. Off. EU, Luxembourg
Eichhorn S, Erfurt S, Hofmann T, Seegmüller S, Németh R, Hapla F (2017) Determination of the phenolic extractive content in sweet chestnut (Castanea sativa Mill.) Wood. Wood Res 62:181–196
EN 113-2 (2021) Durability of wood and wood-based products - test method against wood destroying basidiomycetes - part 2: Assessment of inherent or enhanced durability. European Committee for Standardization, Brussels, Belgium
EN 350 (2016) Durability of wood and wood-based products - testing and classification of the durability to biological agents of wood and wood-based materials. European Committee for Standardization, Brussels, Belgium
Freitas TR, Santos JA, Silva AP, Martins J, Fraga H (2022) Climate change projections for bioclimatic distribution of Castanea sativa in Portugal. Agronomy 12:1137. https://doi.org/10.3390/agronomy12051137
Hama AA, Khwarahm NR (2023) Predictive mapping of two endemic oak tree species under climate change scenarios in a semiarid region: range overlap and implications for conservation. Ecol Inf 73:101930. https://doi.org/10.1016/j.ecoinf.2022.101930
Haupt M, Leithoff H, Meier D, Puls J, Richter HG, Faix O (2003) Heartwood extractives and natural durability of plantation-grown teakwood (Tectona grandis L.) - a case study. Eur J Wood Prod 61:473–474. https://doi.org/10.1007/s00107-003-0428-z
Hosseinihashemi SK, HosseinAshrafi SK, Goldeh AJ, Salem MZM (2016) Antifungal and antioxidant activities of heartwood, bark, and leaf extracts of Robinia pseudoacacia. BioResources 11:1634–1646. https://doi.org/10.15376/biores.11.1.1634-1646
Humar M, Fabčič B, Zupančič M, Pohleven F, Oven P (2008) Influence of xylem growth ring width and wood density on durability of oak heartwood. Int Biodeter Biodegr 62:368–371. https://doi.org/10.1016/j.ibiod.2008.03.010
Huntley JC (1990) Robinia pseudoacacia L. black locust. Silv North Amer 2:755–761
IAWA Committee (1989) IAWA list of microscopic features for hardwood identification. IAWA Bull 10:219–332
Keržič E, Humar M, Oven P, Vek V (2023) Development of extraction methodology for identification of extractive-compounds indexing natural durability of selected wood species. Wood Mat Sci Eng. https://doi.org/10.1080/17480272.2023.2207529
Latorraca JV, Dünisch O, Koch G (2011) Chemical composition and natural durability of juvenile and mature heartwood of Robinia pseudoacacia L. Acad Brasileira Ciênc 83:1059–1068. https://doi.org/10.1590/S0001-37652011005000016
Li G, Xu G, Guo K, Du S (2014) Mapping the global potential geographical distribution of black locust (Robinia pseudoacacia L.) using herbarium data and a maximum entropy model. Forests 5:2773–2792. https://doi.org/10.3390/f5112773
Magel E, Jayallemand C, Ziegler H (1994) Formation of heartwood substances in the stemwood of Robinia pseudoacacia L. II. Distribution of nonstructural carbohydrates and wood extractives across the trunk. Trees - Struct Func 8:165–171
Meyer L, Brischke C, Melcher E, Brandt K, Lenz MT, Soetbeer A (2014) Durability of English oak (Quercus robur L.) – comparison of decay progress and resistance under various laboratory and field conditions. Int Biodeter Biodegr 86:79–85. https://doi.org/10.1016/j.ibiod.2013.06.025
Nadal-Sala D, Hartig F, Gracia CA, Sabaté S (2019) Global warming likely to enhance black locust (Robinia pseudoacacia L.) growth in a Mediterranean riparian forest. Ecol Managem 449:117448. https://doi.org/10.1016/j.foreco.2019.117448
Nicolescu VN, Hernea C, Bakti B, Keserű Z, Antal B, Rédei K (2018) Black locust (Robinia pseudoacacia L.) as a multi-purpose tree species in Hungary and Romania: a review. J Res 29:1449–1463. https://doi.org/10.1007/s11676-018-0626-5
Page D, Ledgard N, Tripti S (2013) The durability of Robinia. Will young trees be suitable for posts? New Z Tree Grower 34:33–35
Pollet C, Jourez B, Hebert J (2008) Natural durability of black locust (Robinia pseudoacacia L.) wood grown in Wallonia, Belgium. Can J Res 38:1366–1372. https://doi.org/10.1139/X07-244
Puchałka R, Dyderski MK, Vítková M, Sádlo J, Klisz M, Netsvetov M, Prokopuk Y, Matisons R, Mionskowski M, Wojda T, Koprowski M, Jagodziński AM (2021) Black locust (Robinia pseudoacacia L.) range contraction and expansion in Europe under changing climate. Glob Change Biol 27:1587–1600. https://doi.org/10.1111/gcb.15486
Rademacher P, Rousek R, Fodor F, Baar J, Koch G, Németh R, Pařil P, Paschová Z, Sablík P, Paul D, Potsch T, Hofmann T (2016) Robinia Wood Research – new innovations for a traditional material. Hardwood Conference 2016. Eco-efficient Resource Wood with special focus on hardwoods, 08-09- September 2016, Sopron, 31–32
Ruppitsch W, Lebow P, Lebow P, Taylor A (2021) Role of Tyloses in the durability of Chestnut Oak. Wood Fib Sci 53:126–146. https://doi.org/10.22382/wfs-2021-14
Sanz M, Sanz M, de Simón BF, Esteruelas E, Muñoz ÁM, Cadahía E, Hernández MT, Estrella I, Martinez J (2012) Polyphenols in red wine aged in acacia (Robinia pseudoacacia) and oak (Quercus petraea) wood barrels. Anal Chim Acta 732:83–90. https://doi.org/10.1016/j.aca.2012.01.061
Schmidt O (2006) Wood and tree fungi. Biology, damage, protection, and use. Springer, Berlin
Schultz TP, Nicholas DD (2000) Naturally durable heartwood: evidence for a proposed dual defensive function of the extractives. Phytochem 54:47–52. https://doi.org/10.1016/S0031-9422(99)00622-6
Schultz TP, Nicholas DD (2002) Development of environmentally-benign wood preservatives based on the combination of organic biocides with antioxidants and metal chelators. Phytochem 61:555–560. https://doi.org/10.1016/S0031-9422(02)00267-4
Sergent T, Kohnen S, Jourez B, Beauve C, Schneider YJ, Vincke C (2014) Characterization of black locust (Robinia pseudoacacia L.) heartwood extractives: identification of resveratrol and piceatannol. Wood Sci Technol 48:1005–1017. https://doi.org/10.1007/s00226-014-0656-x
Singleton VL, Rossi JA (1965) Colorimetry of total phenolics with phosphomolybdic-phosphotungstic acid reagents. Amer J Enol Viticult 16:144–158
Sitzia T, Cierjacks A, de Rigo D, Caudullo G (2016) Robinia pseudoacacia in Europe: distribution, habitat, usage and threats. In: San-Miguel-Ayanz J, de Rigo D, Caudullo G, Houston Durrant T, Mauri A (Eds), European Atlas of Forest Tree Species, Publication office of the European Union, Luxembourg: 166–167. https://w3id.org/mtv/FISE-Comm/v01/e014e79
Smith AL, Campbell CL, Walker DB, Hanover JW (1989) Extracts from black locust as wood preservatives: extraction of decay resistance from black Locust heartwood. Holzforsch 43:293–296. https://doi.org/10.1515/hfsg.1989.43.5.293
Stirling R, Flæte PO, Alfredsen G, Morris PI (2012) Extractives in Norwegian-grown and North American-grown western red cedar and their relation to durability. IRG/WP 12-10762. The International Research Group on Wood Protection
Valette N, Perrot T, Sormani R, Gelhaye E, Morel-Rouhier M (2017) Antifungal activities of wood extractives. Fung Biol Rev 31:113–123. https://doi.org/10.1016/j.fbr.2017.01.002
Vek V, Poljanšek I, Oven P (2019a) Efficiency of three conventional methods for extraction of dihydrorobinetin and robinetin from wood of black locust. Eur J Wood Prod 77:891–901. https://doi.org/10.1007/s00107-019-01430-x
Vek V, Vivod B, Poljanšek I, Oven P (2019b) Content of extractives in bark and wood of black locust (Robinia pseudoacacia L). Acta Silv Ligni 119:13–25. https://doi.org/10.20315/ASetL.119.2
Vek V, Balzano A, Poljanšek I, Humar M, Oven P (2020a) Improving fungal decay resistance of less durable sapwood by impregnation with scots pine knotwood and black locust heartwood hydrophilic extractives with antifungal or antioxidant properties. Forests 11:1024. https://doi.org/10.3390/f11091024
Vek V, Poljanšek I, Oven P (2020b) Variability in content of hydrophilic extractives and individual phenolic compounds in black locust stem. Eur J Wood Prod 78:501–511. https://doi.org/10.1007/s00107-020-01523-y
Vek V, Poljanšek I, Cerc Korošec R, Humar M, Oven P (2022) Impact of steam-sterilization and oven drying on the thermal stability of phenolic extractives from pine and black locust wood. J Wood Chem Technol 42:467–477. https://doi.org/10.1080/02773813.2022.2123520
Vítková M, Müllerová J, Sádlo J, Pergl J, Pyšek P (2017) Black locust (Robinia pseudoacacia) beloved and despised: a story of an invasive tree in Central Europe. Ecol Manag 384:287–302. https://doi.org/10.1016/j.foreco.2016.10.057
Wagenführ R (1999) Anatomie des Holzes. (Anatomy of wood) (In German). DRW, Leinenfelden-Echterdingen
Acknowledgements
Andreas Haisch from Haisch GmbH & Co. KG, Neuweiler, Germany, is acknowledged for providing black locust wood of different origins.
Funding
Open Access funding enabled and organized by Projekt DEAL.
Author information
Authors and Affiliations
Contributions
C.B., H.S., T.K., V.V. and M.H. planned and conducted the experiments, analysed the data, wrote the main manuscript text and illustrated the results. C.M.C.C. conducted the anatomical and durability studies. B.S. did the statistical analysis. A.M.T. planned the experiments and interpreted the results. All authors reviewed the manuscript.
Corresponding author
Ethics declarations
Competing interests
The authors declare no competing interests.
Additional information
Publisher’s Note
Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations.
Rights and permissions
Open Access This article is licensed under a Creative Commons Attribution 4.0 International License, which permits use, sharing, adaptation, distribution and reproduction in any medium or format, as long as you give appropriate credit to the original author(s) and the source, provide a link to the Creative Commons licence, and indicate if changes were made. The images or other third party material in this article are included in the article’s Creative Commons licence, unless indicated otherwise in a credit line to the material. If material is not included in the article’s Creative Commons licence and your intended use is not permitted by statutory regulation or exceeds the permitted use, you will need to obtain permission directly from the copyright holder. To view a copy of this licence, visit http://creativecommons.org/licenses/by/4.0/.
About this article
Cite this article
Brischke, C., Stolze, H., Koddenberg, T. et al. Origin-specific differences in the durability of black locust (Robinia pseudoacacia) wood against wood-destroying basidiomycetes. Wood Sci Technol 58, 1427–1449 (2024). https://doi.org/10.1007/s00226-024-01571-0
Received:
Accepted:
Published:
Issue Date:
DOI: https://doi.org/10.1007/s00226-024-01571-0